Explain the mechanism of setting and hardening of plaster of Paris.
s-Block Elements · Question 269 of 271
Explain the mechanism of setting and hardening of plaster of Paris.
Solution:
Key idea: Plaster of Paris is calcium sulphate hemihydrate, . When mixed with water it takes back water and turns into gypsum, , whose needle-like crystals grow and lock together into a hard mass.
Step 1 — Mix with water: dissolving. When plaster of Paris is mixed with water (typically about 60–80 g of water for every 100 g of plaster) it forms a smooth plastic paste. The hemihydrate is several times more soluble in water than gypsum, so part of it dissolves.
Step 2 — Setting: crystallisation of gypsum. The solution is now supersaturated with respect to gypsum, so small needle-shaped crystals of separate out. As they form, more hemihydrate dissolves, and the process continues. The interlocking needles make the paste stiff within about 5–15 minutes: this is the setting. The change is exothermic, so the paste becomes warm.
Step 3 — Hardening. Over the next hours the gypsum crystals go on growing and interlocking, and the excess water evaporates, so the mass becomes hard and strong: this is the hardening.
Step 4 — Note the expansion and its use. During setting the mass expands slightly (about 1 %), so it fills every detail of a mould, which is why plaster of Paris is used for casts, moulds, statues and surgical bandages. The setting can be speeded up by adding a little common salt or alum, and slowed down by adding borax or glue.
Watch out: If plaster of Paris is overheated during its manufacture (above about 473 K), it becomes anhydrous (dead burnt plaster), which does not set.
Therefore, plaster of Paris sets because the hemihydrate dissolves and recrystallises as interlocking needles of gypsum, , by taking up water; it then hardens as these crystals continue to grow and the excess water dries out, with a slight expansion.