Explain electrometallurgy (Electrolytic reduction) for the extraction of aluminium from its oxide ore.
General Principles and Processes of Isolation of Elements · Question 209 of 228
Explain electrometallurgy (Electrolytic reduction) for the extraction of aluminium from its oxide ore.
Solution:
Key idea: Aluminium is too electropositive to be reduced by carbon at a workable temperature, so pure alumina is reduced by electrolysis of its solution in molten cryolite (the Hall–Héroult process).
Step 1 — Purify the bauxite (Bayer process).
Bauxite is digested with hot concentrated sodium hydroxide solution under pressure. Alumina, being amphoteric, dissolves as sodium aluminate, while iron(III) oxide and other impurities remain undissolved as red mud and are filtered off.
The solution is cooled and seeded with a little freshly made aluminium hydroxide, so aluminium hydroxide crystallises out.
The hydroxide is heated strongly (about 1470 K) to give pure alumina.
Step 2 — Dissolve the alumina in molten cryolite.
Pure alumina melts only at about 2345 K (2072 °C) and molten alumina is a poor conductor. Dissolved in molten cryolite () with a little fluorspar (), it can be electrolysed at about 1250 K (950–980 °C), and the melt conducts well.
Step 3 — Set up the cell.
A steel tank lined with carbon acts as the cathode, and graphite (carbon) blocks dipping into the melt are the anodes. A crust of solid electrolyte and alumina powder covers the melt and reduces heat loss.
Step 4 — Write the electrode reactions.
In the melt the alumina provides aluminium ions and oxide ions. The aluminium ions are reduced at the cathode.
At the anode the oxide ions are discharged, and the oxygen burns the carbon anode to carbon monoxide and carbon dioxide.
Step 5 — Write the overall reaction.
Taking carbon dioxide as the main anode product and balancing the electrons (12 on each side), the overall reaction is written as below.
Step 6 — Collect the aluminium.
Molten aluminium is denser than the electrolyte, so it sinks to the bottom and is tapped off. Fresh alumina is added from time to time, and the anodes are replaced periodically because they are burnt away. The aluminium obtained is about 99.5–99.8 % pure; it can be refined further by the Hoopes electrolytic process.
Note: The process uses about 13–15 kWh of electricity per kilogram of aluminium, so smelters are built where electricity is cheap. The anode gas contains poisonous carbon monoxide and some fluorides, so it is collected and cleaned. The red mud from the Bayer process is strongly alkaline (about 1–1.5 tonnes per tonne of alumina) and is stored in lined ponds.
Therefore, aluminium is extracted by purifying bauxite to alumina (Bayer process), dissolving the alumina in molten cryolite with , and electrolysing it at about 1250 K between a carbon-lined steel cathode and graphite anodes, the overall reaction being .